Ultramarine Blue vs Phthalocyanine Blue in Paints: How to Structure a Fair Comparison

Published

By

A fair comparison of ultramarine blue pigment (Pigment Blue 29) and phthalocyanine blue pigment (Pigment Blue 15) in paint is set up before either blue is judged. Fix six conditions first:

  1. One paint objective: full shade, tint or white correction, plus the service the film must survive.
  2. The exact grade, technical data sheet (TDS) revision and lot of each blue.
  3. One matched basis: equal loading, or a match to an agreed colour target.
  4. One named white, reduction ratio, dispersion route and film build for both blues.
  5. Colour, hiding and exposure methods, with tolerances agreed before anything is measured.
  6. Cost-in-use at the colour target, not price per kilogram.

The two blues come from different chemistry, so neither one wins in every paint. Ultramarine blue is an inorganic sodium aluminosulfosilicate. Phthalocyanine blue is an organic copper complex sold in several crystal forms. A result is valid only for the objective, grade, binder and test conditions it came from. This guide sets out a protocol that procurement and laboratory teams can agree before samples arrive, so the comparison ends in a decision rather than an argument.

Ultramarine blue (Pigment Blue 29) versus phthalocyanine blue (Pigment Blue 15) paint comparison guide with illustrated reddish ultramarine powder, greenish phthalocyanine powder, a blue tint drawdown over a black-and-white hiding chart and a blue painted panel, annotated with objective, matched-basis, white-and-film and cost-in-use checks.
Fix the objective, matched basis, white and film before judging either blue. The powders, drawdown and panel are illustrations, not MPPL grade samples or test results.

Define the paint objective before comparing blues

The question “ultramarine or phthalocyanine?” has no answer until the paint objective is written down. The two pigments are often bought for different jobs. A supplier review of ultramarine in coatings notes that it has traditionally been used to tint white paints, where its blue undertone, its absorbance of yellow wavelengths and its low tinting strength are useful [1]. Copper phthalocyanine, by contrast, is described in the technical literature as by far the dominant blue organic pigment, used extensively in paint, printing ink and plastics [2]. When a buyer asks which of the two to use, the useful first answer is another question: for which paint, which shade and which service?

Without a written objective, each team judges a different property. The colourist looks at hue, the buyer looks at price per kilogram and the plant looks at mill time. All three observations can be correct and still lead to opposite conclusions.

Full shade, tint and white correction are different tests

A full-shade comparison uses the blue as the main colorant. It judges depth, chroma, gloss, transparency or hiding at the production film build. A tint comparison reduces the blue in a white base. It judges tinting strength, the hue of the tint and how clean the pastel looks. A white-correction comparison adds a very small amount of blue to a white or off-white base to neutralise its yellowness. Here the subject is the corrected white, not the blue. The questions are how little blue is needed and what undertone the white takes on.

A pigment that suits one of these objectives may not suit another, so each needs its own comparison. If the same buyer needs a deep blue topcoat and a pastel blue wall paint, plan two comparisons, not one. Write the objective as a single sentence that anyone in the project can check. For example: “A mid-blue tint in our interior acrylic emulsion white base, matched to the approved customer panel and applied by roller.”

Write the service conditions into the objective

The objective should also state where the paint will be used. Record whether it is for interior or exterior use and the durability period expected. Note any contact with acids: industrial atmospheres, acid rain, acid-catalysed binders or binders that release acid as they age. Note contact with alkaline substrates such as fresh masonry, any cleaning chemicals, and the production application method, such as spray, brush, roller or dip.

These conditions decide which grades may enter the comparison at all. Manali Pigments’ ultramarine pigments page states that standard ultramarine pigments are sensitive to acids and should not be assumed suitable for acidic formulations or prolonged acidic exposure. Writing the service into the objective at the start avoids running a full colour comparison on a grade that would be excluded later for a reason everyone already knew.

Name the exact grades, not just the CI names

Colour Index (CI) names identify chemical families, not finished products. Pigment Blue 29 (C.I. 77007) is ultramarine blue. Pigment Blue 15 (C.I. 74160) covers copper phthalocyanine blues in several crystal forms and stabilised versions. A comparison report that says only “ultramarine against phthalo blue” cannot be repeated, because it does not say which two products were tested. The guide to pigment Colour Index names and numbers explains how buyers specify the correct grade, and the Technical Specifications & CI Numbers resource gives the wider context.

Ultramarine blue: one CI name, several grade types

Ultramarine blue is a synthetic sodium aluminosulfosilicate. Its colour comes from sulfur species held inside the aluminosilicate lattice, and Manali Pigments’ product page describes PB 29 as a brilliant reddish-blue shade. Within that one CI name, grades differ in particle size, tinting strength and surface treatment.

Surface treatment matters most for durability. Silica-coated or encapsulated grades are designed to protect the particle from acids. One research study prepared acid-resisting ultramarine blue by a two-step silica coating and judged its acid resistance by immersing the pigment in 10 wt% hydrochloric acid [3]. Supplier literature describes encapsulation aimed at acidic outdoor environments, poorly crosslinked binders and binders that can release acid components as they age [1]. An ultramarine result is incomplete unless it states whether the grade tested was a standard or an acid-resistant type.

Phthalocyanine blue: crystal form and stabilisation

Copper phthalocyanine shows polymorphism. The alpha and beta forms are the important pigment phases. After-treatments are needed not only to convert the crude pigment into a usable pigment form, but also to give it stability towards crystal phase change and flocculation in application [2]. Manali Pigments’ phthalocyanine pigments page describes the alpha grades PB 15, PB 15:1 and PB 15:2 as reddish blue and the beta grades PB 15:3 and PB 15:4 as greenish blue. It lists PB 15:1 as stabilised against crystallisation, PB 15:2 against crystallisation and flocculation, and PB 15:4 against flocculation.

This means an alpha PB 15:1 and a beta PB 15:3 are two different comparators for ultramarine. Choose the one the paint objective calls for, and record the full designation, such as “PB 15:3”, rather than “phthalo blue”. Pigment Green 7, the chlorinated copper phthalocyanine green, belongs to the same chemical family and often appears on the same supplier list. It is a green, though, and it has no place in a blue comparison.

Record grade, TDS revision and lot for each blue

For each candidate, record the supplier, the grade name, the CI name and number, and the physical form: powder or pigment preparation. Record the TDS revision date, the lot number and the date the sample was drawn. If one blue arrives as a powder and the other as a dispersion, the comparison is also testing the dispersion. Either compare both as powders through the same mill route, or both as preparations checked for compatibility. The guide on checking water-based pigment dispersion compatibility covers that second route. For a general overview of how the two families differ, see the earlier article on ultramarine blue vs phthalocyanine blue.

Choose the matched basis: equal loading or equal colour

The basis is the single decision that most often makes a blue comparison unfair. The formulator’s guide to Pigment Blue 29 vs Pigment Blue 15:3 in coatings explains why equal mass does not establish equivalent colour or cost. This section deals with the next step: choosing the basis for the procurement comparison and recording it on every result.

There are two legitimate bases. Equal loading uses the same pigment weight, or the same pigment volume, in each batch. It answers the question “what colour does each blue give at this loading?” It is useful for screening, but it produces two different colours, so it cannot show which blue reaches the target more economically. Equal colour adjusts each blue until it matches an agreed colour target. It answers the question “what loading and formula does each blue need to reach the colour, and what else changes?” This is the basis for a purchasing decision and for cost-in-use. Both can appear in one study, provided every result is labelled with the basis it came from.

Why a relative-strength percentage does not cross families

ISO 787-24:2026 compares the tinting strength of two similar coloured pigments dispersed in an alkyd resin without a drier. It states that it does not apply to coloured pigments that differ greatly in colour on reduction [4]. ASTM D4838, a test method now listed by ASTM as historical, was intended for paints with the same type of vehicle and single-pigment colorants of the same Colour Index name and number [5].

Both methods suit a lot-against-standard check within one grade family, such as comparing a new PB 15:3 delivery with its approved standard. Neither turns a PB 29 against PB 15 comparison into one strength percentage, because the two reduced tints differ in hue, not only in depth. Use relative-strength methods inside each family. Use matching to a colour target across families.

Matching to a target, and when shading is allowed

The target should be a physical reference: an approved panel or a colour standard, measured under the agreed conditions. Each blue is then adjusted to the closest match it can reach. An exact match may not be possible. One ultramarine producer’s brochure states that ultramarines occupy a unique position in colour and that an exact match cannot be achieved by blending other pigment types [6]. Another supplier article describes ultramarine as sitting in a blue colour space that no other pigment or blend can occupy [1]. These are supplier statements, but the comparison plan should allow for them.

Agree two things before matching starts. The first is the colour tolerance that counts as “matched”. The second is whether small additions of a shading pigment, such as a violet or green toner, are allowed to close the gap. If shading is allowed, the shading pigment becomes part of that blue’s formula, its cost and its exposure test. If it is not allowed, record the closest match each blue reached and its colour difference from the target.

Fix the white, reduction ratio and depth of shade

In a tint, the white is half of the result. ISO 8781-1, the ISO method for judging dispersion characteristics from the change in tinting strength, requires the type of white pigment to be agreed. Unless otherwise agreed, it uses a rutile titanium dioxide of type R2 as classified in ISO 591, and it prepares reduced pastes at a depth where reflectance falls between about 15% and 50% [7]. That standard is written for similar pigments, but its discipline carries across: name the white, fix the ratio and work at a depth the instrument can measure well.

Use one named white for both blues

Use the same white pigment grade or the same white base, from the same lot, in the same proportion, for both blues. Whites differ in undertone, scattering power and surface treatment. The hue and apparent strength of a blue tint shift with the white it is reduced in. If the production white base is the real use, test in that base rather than in a laboratory white. For a white-correction objective, the white base itself is the subject, so measure the base without any blue as well, and report how far each blue moves it.

Compare at a defined depth as well as a fixed ratio

At one fixed reduction ratio, two blues of different strength give tints of different depth. Hue judgements made across different depths are unreliable, because a deeper tint can look cleaner or dirtier for that reason alone. ASTM D4838 advised that when sample and standard look widely different at the same ratio of colour to white, another sample should be prepared to bring the two closer in appearance [5].

For a cross-family comparison, set a standard depth, such as the target tint or an agreed standard depth, and adjust each blue’s reduction ratio until it reaches that depth. Then record the ratio each blue needed. That ratio is itself a strength result, measured on your basis rather than the supplier’s.

Read each TDS value on its own basis

Every TDS value carries a basis, and the basis is often in small print. As an example, one Heubach TDS for a PB 15:1 grade states its full-shade reduction with titanium dioxide at a fixed ratio. It reports hue angle at one-third standard depth, calculated to ISO/CIE 11664-4, and the reduction ratio needed to reach that depth to DIN 53235-2. It also names the binder system used for each fastness test [8]. The same sheet states that its information is non-binding and that the processing company must establish the suitability of individual products itself.

The values on that sheet belong to that grade. The lesson is general: two TDS numbers are comparable only when the white, ratio, depth and binder behind them match. When they do not, re-test both blues on your basis. The paint pigment TDS checklist sets out what coatings formulators should compare on a TDS before sampling.

Control dispersion and film preparation

The colour a pigment gives in paint depends on how well it has been dispersed. ISO 8781-1 states that the degree of development of tinting strength depends on the amount of work done in preparing the dispersion. It assesses this by dispersing in stages under specified conditions, in an agreed binder system, and measuring the strength after each stage [7]. Pigments from different families can reach full colour development at different work inputs. If both blues are compared after the same short mill time, the comparison may measure dispersibility rather than colour.

Disperse to a stated endpoint and record the work

Two approaches are valid, as long as the report says which was used. In the first, both blues go through the same mill route and time, which shows colour at a production-realistic work input. In the second, each blue is dispersed to its own endpoint, the stage at which strength stops rising, which shows fully developed colour. Record the mill type, media, charge, time or passes, temperature and fineness reading for each blue.

More work is not always better. ISO 8781-1 notes that a maximum in the strength-development curve can indicate overgrinding, flocculation or recrystallisation [7]. For phthalocyanine blue, that links to the crystal and flocculation stability that after-treatments are designed to provide [2]. For ultramarine, a supplier review lists limited dispersibility among the barriers paint makers have perceived [1], which current grades may or may not show in your mill. Measure it rather than assume it.

Use rub-out to detect flocculation and flooding

In the rub-out test, part of the freshly applied film is rubbed lightly with a finger, and the depth of shade of the rubbed and unrubbed areas is compared. ISO 8781-1 describes it as a way to find out whether pigment separation, such as floating, flooding or flocculation, has occurred [7]. A flocculated blue looks weaker and can shift in hue until it is rubbed. The standard also notes that high-shear application such as spraying gives less rub-out effect than a bar applicator, so a laboratory drawdown and a production spray panel may disagree.

Record the rub-out colour difference and the time between application and rubbing. If one blue shows a strong rub-out, its colour result reflects the dispersion, not the pigment. Fix the dispersion first, through the dispersant, the grade or the mill route, and then compare colour. Keep the film the same for both blues: the same applicator gap, the same chart or substrate, the same flash-off and the same cure. The standard warns that very thick wet films increase the risk of floating and flooding.

Agree how colour will be measured and accepted

Colour data are only comparable when they are produced and judged the same way. Two laboratories can measure the same panels and report different numbers simply because they used different equations or lights.

Specify colour space, equation and tolerance in advance

ISO/CIE 11664-4 specifies how to calculate CIE 1976 Lab* (CIELAB) coordinates, including the correlates of lightness, chroma and hue, and two Euclidean methods for expressing colour difference [9]. ASTM D2244 covers calculating colour tolerances and small colour differences from instrumentally measured coordinates of opaque specimens such as painted panels. For product specification, it requires the purchaser and the seller to agree the permissible colour tolerance between test specimen and reference, and the procedure for calculating it [10]. It cautions that colour differences in different colour-scale systems are not the same and should be compared only within one system. It recommends CIEDE2000 (ΔE00) for small colour differences.

Before measuring, write down the instrument geometry, including whether the specular component is included or excluded. Also record the illuminant and observer, the colour-difference equation, the tolerance and the acceptance rule.

Describe undertone in measured terms too, using hue angle, b* and chroma, rather than words alone. A supplier review describes ultramarine’s undertone as reddish and phthalocyanine blue’s as greenish [1]. Yet the alpha phthalocyanine grades on Manali Pigments’ product page are described as reddish blue. Undertone is a property of the grade, so measure it.

Check metamerism under more than one light

ASTM D2244 calculations are based on daylight illumination. When metamerism is suspected, the standard points to ASTM D4086 for visual confirmation [10]. Two chemically different blues matched to one target will generally have different spectral reflectance curves. A match that holds in daylight can therefore separate under warm indoor lighting or the lights in a retail store.

Measure under at least two illuminants agreed in advance, such as daylight and a warm or retail light source relevant to the market. Then confirm visually in a light booth. If the paint will be tinted at the point of sale or matched to existing stock, this check matters more than a small colour difference under one light.

Measure hiding and transparency with a method that fits the shade

Hiding is where the two families are most often compared unfairly. Each blue can look poor or good depending on whether the objective needs transparency or opacity.

Transparency can be a requirement, not a defect

The Venator ultramarine brochure describes ultramarine as transparent in clear resin. It presents this as a reason to use it in clear lacquers over polished metal, aluminium flake and pearlescent base coats. The brochure adds that ultramarine can be opacified by substituting up to 5% titanium dioxide [6]. The same supplier review that describes ultramarine’s traditional use in white tints lists low opacity among the barriers paint makers have perceived [1].

Whether transparency helps or hurts depends on the objective. For an opaque full-shade blue, any opacifying white must be part of both formulas and part of the colour match. Adding titanium dioxide changes the colour, so match the opacified paint, not the transparent paste.

Use the hiding method’s colour range

ISO 6504-3:2019 determines the hiding power of paint coats of white or light colours with tristimulus values Y and Y10 above 25, applied to a black-and-white chart or a colourless transparent foil [11]. ASTM D2805 determines the hiding power of air-dry coatings with Y tristimulus values above 15% by reflectometry, without reference to a material paint standard [12]. Light tints of either blue can fall within these ranges. A deep full-shade blue film usually falls below them.

For deep shades, agree a practical project method, such as contrast over a black-and-white chart at a stated dry film thickness. Record that it is a project method, not one of those standards. Compare hiding at equal colour rather than equal loading. The loading each blue needs to reach the target changes the total pigment in the film, and that changes hiding.

Test binder compatibility and exposure for the real service

This guide keeps binder and exposure brief. They belong in the qualification plan for the grades that survive the colour comparison. Two points still decide whether the comparison itself is fair.

Acid contact is a grade question for ultramarine

The Venator brochure states that when standard ultramarines face long-term exterior exposure, acid rain can cause the pigment to decompose. The colour change varies with the protection the resin system gives, and the brochure recommends acid-resisting grades for long-term exterior use [6]. A 2026 supplier article adds that ultramarine can decompose in acidic environments, releasing sulfur-containing odours and losing colour [13]. Research on silica-coated ultramarine reports hydrogen sulfide in leaching tests on less protected coating routes [3].

If the paint will contact acids, compare an acid-resistant ultramarine grade, not a standard one, and test it in the real binder. The reverse also applies: do not exclude ultramarine on family reputation when the objective is an interior paint with no acid contact. On the phthalocyanine side, check flocculation and crystal stability in the actual binder and solvent blend [2]. For water-based paints, record the paint pH of both systems, because additives can shift it.

Expose both blues in the same panel build

ISO 16474-2 specifies exposure to xenon-arc light in the presence of moisture, to reproduce the weathering effects of daylight or of daylight filtered through window glass. It leaves specimen preparation and evaluation of the results to other standards [14]. The comparison plan must therefore state the panel build, the exposure cycle and duration, what will be evaluated (for example colour change, gloss retention or chalking) and which result counts.

Build both panels the same way: same binder, white, film thickness and cure. Supplier weathering data are reported in a named system. The Heubach TDS, for example, gives weather fastness for a named water-based automotive system [8]. Data from another binder do not transfer to your paint.

Compare cost-in-use at the colour target

Price per kilogram is not cost per colour. ASTM D4838 noted that tinting strength may be one factor in judging the relative economic value of paints, because pigment concentration contributes to strength in a major way. It added that low tinting strength may lead to an excessively high pigment concentration, which may cause defects in the dry paint film [5]. A 2026 supplier article states that, compared with high-strength organic pigments such as phthalocyanine blue, ultramarine often needs higher loading to reach the same depth of shade, and that this may influence cost-in-use [13]. That is a supplier’s general view. The protocol replaces it with numbers from your own paint.

A worked example with illustrative numbers

The figures below are illustrative. They are not market prices or MPPL data, and they are not mapped to either pigment family. The paint is a 1,000 kg batch of a mid-blue tint. Both candidates are matched to the target within the agreed tolerance, in the same white base and film.

  • Blue candidate 1: price 5.00 currency units per kg. It reaches the target at 9.0 kg and needs 0.4 kg of a shading pigment priced at 30.00 per kg. Pigment cost per batch: 45.00 + 12.00 = 57.00.
  • Blue candidate 2: price 14.00 currency units per kg. It reaches the target at 3.0 kg with no shading. Pigment cost per batch: 42.00.

Candidate 2 costs 2.8 times as much per kilogram but about 26% less per batch at the target. If candidate 1 had reached the target at 6.0 kg without shading, its cost would have been 30.00 per batch, and the ranking would reverse. The arithmetic is simple. The real work is measuring the loading at the target under the controlled conditions described above.

Then add the adjustments that change the total. These include extra white or opacifier needed to reach hiding, and dispersant demand. Include the mill time and energy shown by the work-input record, any premium for an acid-resistant or stabilised grade, and the cost of batch adjustments if one blue needs more correction. Report the result as cost per batch, per litre, or per square metre at the hiding film build. Leave out anything that was not measured rather than estimating it.

Request the documents that make the comparison traceable

A controlled comparison needs controlled samples. For each blue, ask for the current TDS and the basis behind each value: white, reduction ratio, depth and binder. Ask for the safety data sheet (SDS) and for a certificate of analysis (COA) or lot record linked to the sample lot. Ask for a written statement of the grade type, such as standard or acid-resistant ultramarine, or alpha, beta or stabilised phthalocyanine. Keep a retained portion of every sample so that delivery lots can later be compared with what was approved. Ask the supplier which regulatory or market-specific statements apply to the exact grade, paint type and destination market, and obtain them in writing.

Three companion checklists cover these steps in more depth. The paint pigment TDS checklist covers what to compare on the data sheet. The pigment supplier batch consistency checklist covers samples, COAs and retained lots. The pigment manufacturer COA checklist covers approving a production batch. Manali Pigments’ Quality & Compliance page explains that shade is evaluated against the approved reference using the agreed method and tolerance, and invites buyers to ask for grade-specific colour-difference criteria.

Fair comparison grid and decision logic

Use the grid below as the comparison brief. Complete every row for your paint before the first sample is milled, and attach it to every result.

Eight-variable ultramarine blue vs phthalocyanine blue paint comparison grid: what to fix before testing, why it matters and what to record
Variable Fix before testing Why it matters Record
Paint objective Full shade, tint or white correction; interior or exterior service Each objective tests different properties. Write one objective per comparison.
Grade identity CI name, exact grade, TDS revision and lot for each blue PB 29 and PB 15 each cover many grades. Name the grade and lot tested.
Matched basis Equal loading or a match to an agreed colour target Equal weight does not mean equal colour. State the basis on every result.
White and reduction White pigment or base, ratio and depth of shade Strength and hue shift with the white used. Use one named white for both.
Dispersion and film Mill route, endpoint, film thickness, substrate and cure Under-dispersion or flocculation changes colour. Record work input and rub-out.
Colour and hiding Colour space, ΔE equation, illuminants, tolerance and hiding method Results compare only on the same terms. Agree the tolerance before measuring.
Binder and exposure Binder, pH, acid or alkali contact and exposure method Ultramarine acid sensitivity is grade-dependent. Test in the real binder and service.
Cost-in-use Pigment cost per batch at the target, plus adjustments Price per kilogram is not cost per colour. Compare cost at the colour target.
Eight-variable comparison grid for ultramarine blue (PB 29) and phthalocyanine blue (PB 15) in paints covering paint objective, grade identity, matched basis, white and reduction, dispersion and film, colour and hiding, binder and exposure, and cost-in-use.
Compare both blues on one objective, one white and one film. This is a comparison-planning grid, not MPPL grade data or a completed test.

Then use three questions to keep the decision bounded:

  1. Are both blues tested on the same objective, basis and white?
    No → Reset the comparison basis.
    Yes → Proceed to question 2.
  2. Do dispersion, film and measurement terms match for both?
    No → Repeat under controlled conditions.
    Yes → Proceed to question 3.
  3. Do the results meet the tolerance and service criteria agreed in advance?
    No → Record the gap; adjust or reject for that scope.
    Yes → Record a scoped choice and its cost-in-use.

The first question stops a result from comparing two different jobs. The second stops a short mill time, a different film build or a different light from deciding the outcome. The third asks whether the evidence meets a rule written before testing, not a rule adjusted to fit the panels. A No at any stage is a finding about the comparison, not a verdict on either pigment. Once the issue is resolved, return to that question. No route leads to automatic approval.

Decision tree for a fair ultramarine blue versus phthalocyanine blue paint comparison checking the shared objective, basis and white, matched dispersion, film and measurement terms, and pre-agreed tolerance and service criteria before a scoped choice with cost-in-use.
A result holds only for the paint objective tested. This is a decision framework, not completed ultramarine or phthalocyanine test results.

The final record should name the grade and lot of each blue and include the completed grid. It should give the basis, the white and ratio, the work input and rub-out, and the colour results under each agreed illuminant. It should also give the hiding method and result, any binder or exposure findings, the cost-in-use at the target and the next stage, such as a pilot batch or customer approval. A scoped choice for one interior tint does not approve the same grade for an exterior full shade or a different binder. The Pigments for Paints & Coatings pillar explains how pigment selection fits the wider coatings formulation process.

Frequently asked questions

Are ultramarine blue and phthalocyanine blue interchangeable in paint?

No. Pigment Blue 29 is an inorganic sodium aluminosulfosilicate, and Pigment Blue 15 is an organic copper phthalocyanine sold in alpha, beta and stabilised forms. They differ in hue, strength, transparency and chemical behaviour. Either one can replace the other only for a defined paint objective, after a matched comparison shows it meets the agreed colour and service criteria.

Should the two blues be compared at equal loading or at equal colour?

Use equal colour for the purchasing decision. Equal loading shows what each blue gives at the same weight, but it produces two different colours. Matching each blue to an agreed colour target shows the loading, shading and adjustments each one needs, and that is the basis for cost-in-use. Label every result with its basis.

Which white should be used for tint comparisons?

Use one named white for both blues: the same white pigment grade or the same production white base, from the same lot, at the same ratio. ISO 8781-1 requires the white to be agreed and defaults to a rutile titanium dioxide of type R2. If the paint is made in a production white base, test in that base.

Why can two blue paints match in one light and differ in another?

Ultramarine and phthalocyanine blues have different spectral reflectance curves. A match made under daylight can therefore separate under warm indoor or retail lighting. This is metamerism. Measure under at least two agreed illuminants and confirm the match visually in a light booth before accepting it.

How should hiding be compared when one blue is more transparent?

First decide whether the objective needs transparency or opacity. For an opaque paint, include any opacifying white in both formulas and match the opacified paint. Use a hiding method suited to the shade: ISO 6504-3 covers light colours with Y and Y10 above 25, and ASTM D2805 covers Y above 15%. Agree a stated project method for deep full shades.

Is ultramarine blue suitable for exterior paints?

It depends on the grade and the service. Standard ultramarines are sensitive to acids, and suppliers recommend acid-resistant grades for long-term exterior exposure. Compare an acid-resistant grade where acid contact is expected, test it in the real binder, and expose it in the same panel build as the phthalocyanine candidate.

What does cost-in-use mean in a blue pigment comparison?

It is the pigment cost per batch, per litre or per square metre once each blue has been matched to the colour target. It includes any shading pigment, extra white or opacifier, dispersant and mill time the match needs. A blue with a higher price per kilogram can cost less per batch, or more, depending on the loading it needs at the target.

Can shading pigments be used to close the colour gap?

Yes, if this is agreed before matching starts. A small violet or green toner can bring a candidate closer to the target. The shading pigment then becomes part of that blue’s formula, cost and exposure test. If shading is not allowed, record the closest match each blue reached and its colour difference from the target.

What should the final comparison record include?

It should include the paint objective, the grade, TDS revision and lot of each blue, the matched basis, the white and reduction ratio, and the dispersion work and rub-out. It should also give the film build, the colour results under each illuminant, and the hiding method and result. Add any binder or exposure findings, the cost-in-use at the target, and the scope and next stage of the decision.

References

  1. Nubiola, “Ultramarine Blue: A ‘New,’ Unique Color Space for Painting the World Blue”, PCI Magazine, 2006. Supplier review of ultramarine in coatings: traditional white-tinting use, perceived barriers, undertone compared with phthalocyanine blue, and silica encapsulation.
  2. Christie and Abel, “Phthalocyanine blue pigments”, Physical Sciences Reviews, 2021. Review of copper phthalocyanine blue covering polymorphism, the alpha and beta forms, and after-treatments for stability towards crystal phase change and flocculation.
  3. Li, Liu and Sun, “Preparation of Acid-Resisting Ultramarine Blue by Novel Two-Step Silica Coating Process”, Industrial & Engineering Chemistry Research, 2011. Study of silica-coated ultramarine blue tested in 10 wt% hydrochloric acid, with hydrogen sulfide measured in leaching tests.
  4. ISO 787-24:2026 — General methods of test for pigments and extenders — Part 24: Photometric methods for determining the relative tinting strength of coloured pigments and the relative scattering power of white pigments. Official record for comparing the tinting strength of two similar coloured pigments in an alkyd resin; it does not apply to pigments that differ greatly in colour on reduction.
  5. ASTM D4838-88(2010) — Standard Test Method for Determining the Relative Tinting Strength of Chromatic Paints. Historical ASTM method for paints with the same vehicle type and single-pigment colorants of the same Colour Index name and number; discusses tinting strength and economic value.
  6. Venator, ULTRAMARINE pigments brochure (English). Producer brochure covering transparency in clear resins, opacifying with titanium dioxide, colour correction of whites, and acid-resisting grades for long-term exterior exposure. Values in the brochure belong to that producer’s grades.
  7. ISO 8781-1:1990 — Pigments and extenders — Methods of assessment of dispersion characteristics — Part 1: Assessment from the change in tinting strength of coloured pigments. Official record for staged dispersion in an agreed binder, reduced pastes with an agreed white, and strength development as a measure of dispersibility.
  8. Heubach, MONOLITE Blue CSN-N (Pigment Blue 15:1) technical data sheet. Example of how a TDS declares its basis: reduction ratio with titanium dioxide, standard depth, colour calculation and the binder used for each test. Values belong to that grade.
  9. ISO/CIE 11664-4:2019 — Colorimetry — Part 4: CIE 1976 Lab* colour space. Official record for calculating CIELAB coordinates, the correlates of lightness, chroma and hue, and Euclidean colour differences.
  10. ASTM D2244-25 — Standard Practice for Calculation of Color Tolerances and Color Differences from Instrumentally Measured Color Coordinates. Practice for colour tolerances of opaque specimens such as painted panels; purchaser and seller agree the tolerance and calculation procedure.
  11. ISO 6504-3:2019 — Paints and varnishes — Determination of hiding power — Part 3: Determination of hiding power of paints for masonry, concrete and interior use. Official record for hiding power of white or light-coloured paint coats with tristimulus values Y and Y10 above 25.
  12. ASTM D2805-11(2023) — Standard Test Method for Hiding Power of Paints by Reflectometry. Instrumental hiding-power method for air-dry coatings with Y tristimulus values above 15%, without a material paint standard.
  13. Fineland Chem, “Ultramarine Blue: Advantages, Limitations and Why It Remains a Valuable Industrial Pigment”, 2026. Supplier article on ultramarine loading relative to high-strength organic blues, cost-in-use and acid decomposition.
  14. ISO 16474-2:2013 — Paints and varnishes — Methods of exposure to laboratory light sources — Part 2: Xenon-arc lamps. Official record for xenon-arc exposure with moisture; specimen preparation and evaluation are covered by other standards.

Explore phthalocyanine blue pigments for your paint comparison

Manali Pigments Private Limited manufactures its pigment categories in-house, including ultramarine and phthalocyanine pigments. Which blue suits your paint still depends on the objective, the grade, the white and binder, the film and the service it has to meet. Review the Phthalocyanine Blue & Green product information first, and the Ultramarine Pigments page for the other side of the comparison. Then bring your paint objective, colour target, white base, binder, film build, exposure needs and document requirements into a grade-specific discussion.

The link below opens the Phthalocyanine Pigments product page. There you can review alpha, beta and stabilised blue grades and discuss the sample and documents your paint comparison needs.